™ Scotch-Weld™
Epoxy Adhesive
DP405 Black
3M™ Scotch-Weld™ Epoxy Adhesive DP405 Black is supplied in dual syringe plastic
duo- pak cartridges as part of the 3M™ EPX™ Applicator System. The duo-pak
cartridges are supplied in 37 ml, 200 ml and 400 ml configurations. To use the EPX
cartridge system simply insert the duo-pak cartridge into the EPX applicator. Next,
remove the duo-pak cartridge cap and expel a small amount of adhesive to be sure both
sides of the duo-pak cartridge are flowing evenly and freely. If simultaneous mixing of
Part A and Part B is desired, attach the EPX mixing nozzle to the duo-pak cartridge
and begin dispensing the adhesive.
When mixing Part A and Part B manually the components must be mixed in the
ratio indicated in the typical uncured properties section of this data sheet. Complete
mixing of the two components is required to obtain optimum properties.
Two-part mixing/proportioning/dispensing equipment is available for intermittent or
production line use. These systems are ideal for line uses because of their variable
shot size and flow rate characteristics and are adaptable to most applications.
Apply adhesive to clean, dry surfaces, joint parts and secure until adhesive sets (see
rate of strength build up).
Surface Preparation The following surface preparations were used for substrates described in this Technical
Data Sheet.
A. Aluminum Etch
Optimized FPL Etch - 3M (test method C-2803)
1. Alkaline degrease – Oakite 164 solution (9-11 oz./gallon water) at 190°F ± 10°F
(88°C ± 5°C) for 10-20 minutes. Rinse immediately in large quantities of cold
running water (3M test method C-2802).
2. Optimized FPL Etch Solution (1 liter):
Material Amount
Distilled Water 700 ml plus balance of liter (see below)
Sodium Dichromate 28 to 67.3 grams
Sulfuric Acid 287.9 to 310.0 grams
Aluminum Chips 1.5 grams/liter of mixed solution
To prepare 1 liter of this solution, dissolve sodium dichromate in 700 ml of distilled
water. Add sulfuric acid and mix well. Add additional distilled water to fill to 1
liter. Heat mixed solution to 66 to 71°C (150 to 160°F). Dissolve
1.5 grams of 2024 bare aluminum chips per liter of mixed solution. Gentle
agitation will help aluminum dissolve in about 24 hours.
To FPL etch panels, place them in the above solution at 150 to 160°F (66 to 71°C)
for 12 to 15 minutes.
Note: Review and follow precautionary information provided by chemical suppliers
prior to preparation of this etch solution.
3. Rinse immediately in large quantities of clear running tap water.
Handling and
Application
Information
Directions for Use